Revista de la Facultad de Ingeniería Universidad Central de Venezuela
versão impressa ISSN 0798-4065
Rev. Fac. Ing. UCV v.20 n.2 Caracas maio 2005
Mechanical, thermal and morphological behavior of ps/pp blends: High Doses (70-1300 kgy) of Gamma Irradiation
ALBANO C. 1,2,*, REYES J. 2, ICHAZO M. N. 3, GONZÁLEZ J. 3, HERNÁNDEZ M.3
1Laboratorio de Polímeros, Centro de Química, Instituto Venezolano de Investigaciones Científicas (IVIC), Apdo 21827, Caracas 1020-A, Venezuela .
2Universidad Central de Venezuela, Facultad de Ingeniería, Escuela de Ingeniería Química, Los Chaguaramos, POBox: 48146, Caracas 1041A, Venezuela.
3Universidad Simón Bolívar, Departamento de Mecánica, Caracas 1080A, Venezuela.
*Corresponding Author: calbano@ivic.ve/ albanoc@camelot.rect.ucv.ve
ABSTRACT
A study of the effect of high doses (70-1300 kGy) of gamma irradiation on mechanical, morphological and thermal behaviors, at room temperature and in the presence of oxygen, occurring in the polystyrene/polypropylene blend (80/20) with and without compatibilizer (block styrene-butadiene-styrene (SBS)) at 7.5 wt.% is required to solve different problems related to the radiation stability of articles made of polymers and purposeful radiation-induced modifications on polymeric materials. The effect of gamma irradiation on the tensile behavior of the PS/PP blend (80/20) without and with SBS points to a deterioration of the mechanical properties of the blends due to the scission and crosslinking reactions resulting from irradiation. This deterioration is confirmed based on the morphology of the fracture surface, melt flow, PP crystallinity and PS glass transition temperature in the blends.
MECHANICAL, THERMAL AND MORPHOLOGICAL BEHAVIOR OF PS/PP BLENDS: HIGH DOSES (70-1300 KGY) OF GAMMA IRRADIATION
RESUMEN
En el presente trabajo se estudia el efecto de altas dosis (70-1300 kGy) de radiación gamma a temperatura ambiente y en presencia de oxígeno sobre el comportamiento mecánico, morfológico y térmico de mezclas de Poliestireno/Polipropileno (PS/PP, 80/20) con y sin compatibilizante (copolímero en bloque estireno-butadieno-estireno SBS) a la composición de 7.5% en peso; con el fin de tratar de resolver los problemas relacionados con la estabilidad frente a la radiación de artículos manufacturados con estos polímeros, y al mismo tiempo analizar las modificaciones inducidas por la radiación en estos materiales poliméricos. Con respecto al comportamiento tensil de las mezclas de PS/PP con y sin SBS inadiados, se tiene que ocurre un deterioro de las propiedades mecánicas debido a las reacciones de ruptura y entrecruzamiento que se producen. Este deterioro se confirma a través de los estudios de la superficie de factura, el indice de flujo, la cristalinidad del PP y la temperatura de transición vítrea del PS de los componentes de las mezclas.
Recibido: Julio 2003 Recibido en forma final revisado: Mayo 2005
INTRODUCTION
The use of radiation in the processing of polymers is gaining more and more interest because it can be suggested as an alternative to the traditional chemical methods [1] to modify the molecular structure of polymers. The possibility of processing the final shape of the polymeric material in the solid state opens up new opportunities to obtain materials with well-tailored properties.
Detailed studies on g-irradiated materials are needed to increase the variety of polymer blends. Ionizing radiation induces chemical reactions in polymers, which result in changes in both molecular structure and macroscopic properties [2-4].
The study of the mechanical, thermal and morphological behavior of the blends of PS/PP (80/20) and PS/PP (80/20) with SBS, at 7.5wt.% composition respect to the blends, irradiated with gamma rays from a 60Co source at a dose rate of 4.8 kGy/h and at high integral doses of 0-70-400-800-1300 kGy, in the presence of air and at room temperature, is necessary to solve different problems related to the radiation stability of polymeric articles and purposeful radiation-induced modifications of polymeric materials.
EXPERIMENTAL
The polymers used in this study were polypropylene PP J300 (MFI: 1.6g/10min), supplied by Propilven, polystyrene PS supplied by EstiZulia (MFI: 2.3g/10min) and a triblock copolymer based on styrene-butadiene-styrene (SBS), Styrolux, (r: 1.08 g/cm3, 48% wt.% of styrene) supplied by Bash. To inhibit or delay the decomposition process, Recyclostab 811, supplied by Ciba-Geigy, was added to the polymer as an additive.
The blends were prepared in 80/20 wt.%, PS/PP. A styrene-butadiene-styrene copolymer, 7.5wt.% respect to the blend, was used as a modifier in the blend. These choices were based on previous research on the mechanical behavior of this blend with and without compatibilizer [5]. The blends were prepared in a W&P intermeshing co-rotating twin-screw extruder and mixing took place with a temperature profile of 150, 190, 210, 215 and 210 C and at a screw speed of 110 rpm. Then, the specimens were compression molded at 35 MPa and 210 C. The blend of PS/PP with SBS is mixed in the same way and under the same extrusion and molding conditions.
The samples were irradiated with g rays at integral doses of 70, 400, 800 and 1300 kGy using a dose rate of 4.8 kGy/h in the presence of air, at room temperature, with a 60Co source supplied by the Venezuelan Institute of Scientific Research (IVIC). The experimental measurements were taken after thirty days of storage in the presence of air.
The effect of gamma irradiation on the mechanical properties (elongation at break and tensile strength) was studied using an Instron Tensile tester (model 1131-C6) with a crosshead rate of 25 mm/min according to ASTM D-638. Each experimental point represents an average over at least ten samples irradiated under identical conditions. The notched Izod impact test was performed at room temperature in a Zwick machine according to ASTM D-256. A Hitachi S-2400 scanning electron microscope (SEM) was used to observe morphology of the samples.
Differential scanning calorimetry (Mettler Toledo, DSC 821) was used to observe glass transition temperature and melting behavior (second heating). Three tests were carried out for each sample and the temperature difference was less than 1°C. Nitrogen was used as a dragging gas.
A Davenport Extrusion Plastometer was used to obtain data for the calculation of the MFI of each material. Procedures were performed according to ASTM D 1238, 200 °C and 5kg. Each sample was tested three times and the results averaged. The standard deviations were no higher than 10%.
RESULTS AND DISCUSSION
Table 1 includes the values of tensile and impact properties of the neat polymers (PP, PS) and of the blends PS/PP and PS/PP with SBS, without irradiation and irradiated at 70 kGy. The results in this Table 1 show that PP presents a decrease in impact strength (IS) and elongation at break (eB) what implies a dominant degradative chain scission process [6] PDS PP/SBS . On the contrary, the increase detected in the breaking strength (sB), approximately 25%, is due to a light crosslinking in PP at low irradiation doses. This variation confirms the results observed by Chapiro [7], that irradiated PP has a ratio of 1.6 scission for every crosslink formed. Also, Varada Rajulu et al. [8] demonstrated by means of FTIR studies that at low doses, PP bands change towards lower frequencies, which is indicative of crosslinking reactions. Young's modulus, in turn, does not show significant variations.
On the other hand, PS behavior shows no significant changes in mechanical properties within this dose interval and this is due at least for the following reasons: the presence of the benzene ring in PS, meaning a high resistance to degradation [9]; and the high intermolecular forces that minimize changes, at temperatures below the glass transition temperature (<70C), from radiation-induced crosslinking and scission, which also render the strength properties very insensitive to radiation at low doses [10].
Table 1: Mechanical behavior of PP, PS, PS/PP and PP/PS-St., with and without irradiation at 70 kGy
| Samples | IR (J/m) | sB (MPa) | eB (%) | E ( MPa) | ||||
| 0 kGy | 70 kGy | 0 kGy | 70 kGy | 0 kGy | 70 kGy | 0 kGy | 70 kGy | |
| PP | 20.7±1.5 | 8.8±2.3 | 22.5±3.5 | 30.1±2.1 | 14.8±0.8 | 11.3±1.9 | 600±100 | 674±60 |
| PS | 4.3±0.6 | 5.0±0.9 | 13.4±0.8 | 11.8±1.1 | 1.9±0.2 | 1.6±0.2 | 1041±73 | 969±89 |
| PS/PP | 2.4±0.9 | 2.5±0.9 | 11.2±1.3 | 13.3±2.0 | 1.4±0.2 | 1.6±0.3 | 735±61 | 810±112 |
| PS/PP/SBS | 15.1±2.3 | 13.8±1.4 | 29.2±1.8 | 25.5±1.8 | 4.8±0.3 | 4.1±0.3 | 778±54 | 871±70 |
In the case of the blends (PS/PP and PS/PP with SBS), variations are not significant. Thus high radiation doses are required to produce any noticeable change.
When irradiation doses are high, IS (Impact Strength) value for PP (Table 2) decreases in 50% at integral irradiation doses of 1300 kGy (4.3J/m) with respect to the value at 70 kGy (8.8J/m). In the case of PS, the decrease in IS (Table 2) shows a similar percentage (50%) in the dose interval ranging between 70 and 400 kGy, changing from 5.0 J/m to 3.1 J/m. At higher doses (>400kGy) the decrease is slower (" 2.5 J/m).
Elongation at break (eB) and tensile strength (sB) of PP (Tables 3 and 4)) show a very marked decrease, from 88% to 50%, within the interval between 70 to 400 kGy, respectively. At higher irradiation doses, the decrease is relatively slower. This behavior is due to the fact that the degradative process is very fast at those doses (70-400 kGy), because during the degradation process, the formation of peroxy radicals in the amorphous regions appears to be the primary cause of the loss of physical properties. When sufficient number of tie molecules between crystallites are cut throughout this chain scission process, elongation at break, tensile strength and impact strength are reduced dramatically and a catastrophic failure results.
The behavior of these properties (eB and sB) for PS (Tables 3 and 4)) is different from that of PP. When the integral irradiation dose goes from 70 to 400 kGy, an increase of approximately 60% is observed and then a progressive decrease at higher irradiation doses. This behavior can be explained based on the fact that crosslinking processes begin within this range and this process and the scission reaction one continue at higher irradiation doses (400-1300kGy). These results are in agreement with those of Browmer et al. [11] who observed a slight decrease in the tensile strength of PS at doses greater than 800 kGy; this decrease was attributed to chain scission on the surface of the sample. Bikales et al. [12] demonstrated that when tensile polystyrene specimens were exposed to high gamma radiation in the presence of air, chain scission predominated on the surface whereas crosslinking did inside the sample. Varada Rajulu et al. [8] also demonstrated that irradiated PS formed crosslinkings. In the PS chemical structure, those possible sites where these crosslinkings can exist are in the form of an a-carbon atom to which the phenyl group is attached; in addition, the removal of a hydrogen atom facilitates crosslinking on this site. Schnabel et al. [13] also demonstrated that PS at irradiation doses of 600 kGy and at a dose rate of 2.4 kGy/h crosslinked.
IS of the compatibilized and non-compatibilized samples at high irradiation doses (Table 2) present the same decreasing behavior as the neat polymers, but in a more drastic fashion, that is, variation went from 2.5 J/m and 13.8 J/m at 70 kGy to <1.0 J/m and 1.8 J/m at 1300 kGy, respectively. It is worth mentioning that IR values are lower for the PS/PP blend without compatibilizer when compared with the same blend compatibilized with Styrolux.
Table 2: Impact Strength (J/m) of PP, PS, PS/PP and PP/PS-St, at different radiation doses
| Irradiation dose | PP | PS | PS/PP | PS/PP/SBS |
| 70 kGy | 8.8±1.2 | 5.0±0.9 | 2.5±0.9 | 13.8±2.3 |
| 400 kGy | 6.1±1.1 | 3.1±0.6 | 1.1±0.3 | 4.3±0.9 |
| 800 kGy | 5.7±0.9 | 2.3±0.6 | <1.0 | 2.5±0.9 |
| 1300 kGy | 4.3±0.6 | 2.5±0.6 | <1.0 | 1.8±0.6 |
Table 3: Elongation at break (%) behavior of PP, PS, PS/PP and PS/PP-St., at different radiation doses.
| Irradiation dose | PP | PS | PS/PP | PS/PP/SBS |
| 70 kGy | 11.2±1.9 | 1.4±0.2 | 2.2±0.3 | 4.1±0.3 |
| 400 kGy | 1.3±0.2 | 2.4±0.2 | 3.2±0.3 | 1.2±0.2 |
| 800 kGy | 1.8±0.2 | 2.2±0.3 | 2.2±0.1 | 1.5±0.3 |
| 1300 kGy | 2.3±0.2 | 1.2±0.2 | 1.9±0.1 | 1.2±0.2 |
Table 4: Tensile strength (MPa) behavior of PP, PS, PS/PP and PS/PP-St., at different
| Irradiation dose | PP | PS | PS/PP | PS/PP/SBS |
| 70 kGy | 11.2±1.9 | 1.4±0.2 | 2.2±0.3 | 4.1±0.3 |
| 400 kGy | 1.3±0.2 | 2.4±0.2 | 3.2±0.3 | 1.2±0.2 |
| 800 kGy | 1.8±0.2 | 2.2±0.3 | 2.2±0.1 | 1.5±0.3 |
| 1300 kGy | 2.3±0.2 | 1.2±0.2 | 1.9±0.1 | 1.2±0.2 |
Table 5: Tensile modulus (MPa) behavior of PP, PS, PS/PP and PS/PP-St., at different radiation doses.
| Irradiation dose | PP | PS | PS/PP | PS/PP/SBS |
| 70 kGy | 674±60 | 969±89 | 810±112 | 871±70 |
| 400 kGy | 835±136 | 944±91 | 818±124 | 791±49 |
| 800 kGy | 875±52 | 960±42 | 887±75 | 843±65 |
| 1300 kGy | 889±60 | 1143±96 | 859±68 | 898±104 |
Table 6: MFI (g/10min±0.1) of the blends of PS/PP with and without SBS. (MFI of the PP alone: 4.06 g/10 min, ( * melt fractured))
| Radiation doses (kGy) | PS/PP with St. | PS/PP |
| 70 | 1.7 | 15.5 |
| 400 | 3.4 | 10.2 |
| 800 | * | * |
| 1300 | * | * |
The behavior of elongation at break and tensile strength of the PS/PP blend without compatibilizer (Tables 3 and 4) is similar to that of PS, whereas values of these properties for the compatibilized PS/PP blend (Tables 3 and 4) show a decreasing behavior. This is due to some factors:
-The oxidation process of SBS as a result of the polybutadiene blocks in its structure, because samples take a yellowish coloration due to irradiation and the chain scission occurring in the butadiene block. Scott [14] postulates that the C-H bond of styrene (styrene block) is more stable than the C-H bond of the allyl group of butadiene due to an induction effect (butadiene block). The steric hindrance of the phenyl group and delocalization of radicals by the allyl group (CH2=CH2-CH3 " CH2=CH-CH2) imply that the oxidation process begins in the rubbery phase of SBS (allyl group). Vishwa Prasa & Singh [15] report that SBS irradiation produces epoxy dews and alcohols that decompose into carbonyl products.
-The chain scission reactions occurring in PS and in the SBS styrene block of the sample surface result in deterioration of these properties.
-Scission in the linkage between PS and the butadiene block of SBS.
In addition, studies conducted by Vishwa Prasas & Singh [15] indicate that a phase separation (styrene and butadiene) takes places in SBS due to degradation, forming microcracks that result in a deterioration of mechanical behavior. Schnabel et al. [13] demonstrated that at high irradiation doses ( >1000 kGy) in SBS intermolecular crosslinks were generated, whereas at low doses, instaurations are produced in the butadiene part of the copolymer. Dole [16], in turn, reported that at very high irradiation doses, styrene-butadiene-based copolymers showed crosslinking, hardening and embrittlement of the rubber phase, thus resulting in a sudden decrease in mechanical properties.
The values of Young's modulus of the PS alone, as well as those of the blends (Table 5), show that no significant variations occur at the irradiation dose.
In addition, the behavior exhibited by these mechanical properties (Tables 3 and 4) is confirmed by the values of the melt flow index (Table 6) obtained at the different irradiation doses studies.
In the case of the PS/PP blends with SBS an increase in MFI from 1.71 to 3.36 g/10 min is observed within 70-400 kGy, which is in agreement with Schnabel et al. [13] who reported that SBS at high doses produces crosslinking reactions and, at low doses, insaturations in the butadiene part giving rise to chain scission [14]. Regarding PS, it has been stated in this work that crosslinking take place inside the sample. This has been confirmed by means of photos (Figure 1) taken to the extrude in the MFI study. According to this, at high doses the samples cannot melt completely due to the crosslinking reactions resulting from irradiation. In the PP/PS samples a predominance of crosslinking reactions is observed, resulting from a MFI decrease (Table 6), which confirms the results of the kinetic analysis of mechanical properties as well as their behavior. In addition, as irradiation dose was increased, the extrude did not melt completely, as shown in Figure 3.

Figure 1: Photos taken to the extrude in the MFI Study: a) PS/PP, b) PS/PP with SBS, at 800 kGy.
The mechanical behavior analyzed is in agreement with morphologies observed for PP, PS and blends in Figures 2 and 3, at irradiation doses of 70 kGy and 800 kGy. The deterioration of the fracture surface of PP and PS, when they are subjected to high irradiation doses (800 kGy), can be observed in Figure 2, being this a result of the increasing fragility of the samples. In the case of the PS/PP blends with and without compatibilizer (Figure 3), micrographs show that irradiation has not improved interface interaction. Moreover, on blends with a compatibilizer it is observed a significant change in the fracture surface which could be due to the effect of the g-radiation on the polymers and copolymer composing the blends. Any change in the behavior of the blends (PS/PP and PS/PP with SBS) after irradiation are therefore likely to be a consequence of crosslinking and chain scission.
The PS behavior is supported by the behavior observed in glass transition temperature of this polymer (Figure 4a), which remains constant approximately in the interval 0-70 kGy, increases from 100 C up to 105 C within the dose range between 70 and 400 kGy, and then stays constant at 1300 kGy. This is indicative of a crosslinking process in this irradiation dose range, which is well documented [17], as demonstrates the yellowish coloration of the samples. On the other hand, PP fusion temperature (Figure 4b) shows a continuous decrease, varying from 159 C at 0 kGy to 152 C at 70 kGy, and to 139 C at 1300 kGy. Similar behavior is observed in PP in the blends under study (Figure 5). These results confirm that within this range of high irradiation doses, PP shows a high oxidative degradation (chain scission). In addition, Tg of PS in the blends shows no significant increases, the variation being 2 C (Figure 5).
On the other hand, crystallinity of the blends (Table 7) is found to decrease as a function of the irradiation dose, which is related to crosslinking reactions induced by that radiation what decrease the rate of the transport of crystallizable segments of PP to the crystallization front during the cooling process of these blends in the DSC. Variations in crystallinity of PP alone are not observed, although this polymer shows a degradative process of chain scission with the irradiation dose. According to Dole [16], doses higher than 1000 kGy are required to detect variations in PP crystallinity.
The scission and crosslinking processes produced in PP, PS and their blends [12], are due to: 1) tertiary polystyryl radicals, which are found initially by gamma irradiation because of scission of the C-H bond, 2) the ciclohexadienyl radicals that have also been found and are attributed to the addition of a hydrogen radical to the phenyl ring. Close to room temperature and in the absence of oxygen, polystyryl radicals react by crosslinking, which should happen inside the specimens due to the low oxygen concentration and its slow diffusion inside the sample; and 3) the alkyl radical in PP, which transforms into a peroxide radical. According to Gugumus [18], PP hydroperoxides, in the solid phase, can interact with two adjacent carbon atoms of the polymer chain and the result would be chain scission and the formation of carbonyl groups, thus resulting in a bimolecular kinetic mechanism involving intramolecular and intermolecular hydroperoxide decomposition reactions.

Figure 2: Micrographs of the PP irradiated at <70kGy (a) and 800 kGy (b) and PS irradiated at <70kGy (c) and 800 kGy (d).
Figure 3: SEM micrographs of the PS/PP blend without compatibilizer irradiated at 70 (a) and 800 KGy (b)and PS/PP with SBS irradiated at 70 (c) and 800 KGy (d).

Figure 4: Thermal behavior: (a) glass transition Temperature of PS and (b) second heating of PP, at different radiation dose.


Figure 5: Thermal behavior (second heating) of PS/PP and PS/PP-St., at different radiation dose.
Tabla 7: Crystallinity of PP alone and of the blends as a function of the irradiation dose
| Irradiation dose | Crystallinity | ||
| PP | PS/PP | PS/PP/SBS | |
| 0 kGy | 0.45 | 0.36 | 0.36 |
| 70 kGy | 0.42 | 0.34 | 0.39 |
| 400 kGy | 0.41 | 0.30 | 0.22 |
| 800 kGy | 0.43 | 0.21 | 0.18 |
| 1300 kGy | 0.42 | 0.21 | 0.20 |
CONCLUSIONS
-The effect of g irradiation on the tensile and impact behavior of PS/PP blend without and with SBS indicates that the blends present a high degradation resistance at low doses (£70 kGy).
-When the irradiation dose is high (70kGy £ DI £ 1300kGy), mechanical properties of the homopolymers (PS, PP) deteriorate. In the case of PP, this behavior is due to the scission reactions resulting from the irradiation applied. On the contrary, the PS tensile and impact behavior is the result of the scission processes on the surface of the sample and the crosslinking processes inside it. These degradation processes are confirmed by the behavior of glass transition temperature of PS and fusion temperature of PP.
-Mechanical deterioration of the blends of PS/PP with and without SBS is due to the chain scission and crosslinking reactions produced in the components of the blends as a result of irradiation.
-In the PS/PP blends with and without SBS in the interval 70-1300 kGy, MFI values demonstrated that crosslinking process prevails in the blends within the dose interval analyzed, being this effect more marked for the blends with SBS. This degradative behavior gave origin to a sudden decrease in the properties at the break point (sB and eB).
-Morphology of the fracture surface of the blends is indicative of a change that could be due to the crosslinking process; this effect is more pronounced in the blend of PS/PP with SBS.
-The decrease in PP crystallinity in the irradiated blends of PS/PP with and without SBS is related to the fact that the crosslinking hinders the transport of PP crystallizable segments to the crystallization front, thus affecting the tensile behavior of the blends under study.
REFERENCES
1. SPADARO G., VALENZA A., POLYM. DEG. STAB., 67, 449 (2000).
2. CHANG Z., LAVERNE J., J. Polym. Sci., Part A: Polym. Chemistry. 38, 1656-1661 (2000).
3. ZHANG X.C., BUTLER M. F., CAMERON R. E., Polym. Inter., 48, 1173 (1999).
4. KADIR Z., YOSHII F., MAKUUCHI K., ISHIGAKI I., Polymer, 30, 1425(1989).
5. SCIAMANNA R. ALBANO C., ARRIBAS G.,TECHNICAL Conference Antec'99, New York, USA, Vol III, 3916 ( 1999).
6. PERERA R., ALBANO C., GONZÁLEZ J.,SILVA P., ICHAZO M., Polym. Deg. Stab., (2004) in press.
7. CHAPIRO A., Radiation Chemistry of Polymeric system. London: Interscience (1962).
8. VARADA RAJULU A., LAKSHMINARAYANA REDDY R., AVASTHI D. K., ASOKAN K., Radiation Effects & Defects in Solids, 152, 57 (2000).
9. CHIPARA M. I., BARB D., COJOCARU M., TUDOR D., CHIPARA M. D., ROGALSKI M., Polym. Degrad. Stab., 37, 61(1992).
10. LEVEDEV E. V., in Physic-Chemistry of Multi-component Polymer System, J. Lipatov, Ed. Nauk, Dumka, Kiev, vol 2, 1986.
11. BROWMER T. N., COWEN L. K., O´DONNELL J. H., WINSUR D. J., J. Appl. Polym. Sci., 24, 425 (1979).
12. BIKALES M., O. MENGLES, Encyclopedia of Polymer Science and Engineering, Vol 16, Second Edition, A. Wiley-Interscience Publication. John Wiley & Sons, Canada (1989).
13. SCHNABEL W., LEVCHIK G. F.,WILKIE C. A., JIANG D. D., LEVCHIK S. V., Polym. Deg. Stab., 63, 365 (1999).
14. SCOTT G., Atmospheric Oxidation and Antioxidants, Elsevier, London, 1965, pag. 25.
15. VISHWA PRASAD A., SING. R. P., J. Appl. Polym. Sci., 70, 637 (1998).
16. DOLE M., "The Radiation Chemistry of Macromolecules", New York: Academic Press, 1972.
17. GRASSIE N., WEIR N. A., J. Appl. Polym. Sci., 9, 999 (1965).
18. GUGUMUS F., Polym. Deg. Stab., 74, 327 (2001).